Salt lake brine is the lowest-cost lithium resource in the world and the hardest to process selectively, because lithium is a minor constituent. A typical brine contains 100-2000 mg/L lithium against 50-100 g/L sodium and, in some Chinese lakes, 10-30 g/L magnesium. Any separation process must therefore achieve a lithium-to-sodium selectivity in the thousands, and that requirement rules out simple ion exchange and points to materials with a lattice that accommodates lithium specifically.
The established answer is adsorptive separation on lithium-selective inorganic materials, usually aluminium-based layered double hydroxides or titanium-based ion sieves such as H2TiO3 and H4Ti5O12. These materials have a crystal structure with sites sized for the lithium ion, and they operate by a topotactic mechanism: lithium enters the lattice, displaces protons, and is later eluted with dilute acid. Because the selectivity is structural rather than electrostatic, a good material achieves lithium-to-sodium separation factors above 1000 and lithium-to-magnesium above 100, which no organic ion exchange resin approaches.
In practice the inorganic powder is formed into granules or beads, often by granulating with a binder or by embedding in a polymer matrix, so it can be used in a packed column. That shaping step is where most of the engineering difficulty lies: the binder must not block the active sites, the granule must survive repeated acid elution and thermal cycling, and the pressure drop must stay within what a moving-bed contactor can handle. Plants that succeed commercially tend to be the ones that solved the granulation, not the ones that found the best chemistry.
The flowsheet around the adsorbent matters as much as the adsorbent itself. Raw brine is first clarified and, where magnesium is high, partially de-magnesium by liming, because magnesium hydroxide precipitation inside the column would blind it. The brine then passes through the adsorption beds at a few bed volumes per hour, and loaded beds are eluted with 0.1-0.5 M hydrochloric acid to produce a lithium chloride solution at 1-10 g/L. That solution still carries sodium, potassium, boron and residual magnesium, so it goes to a purification train before carbonate or hydroxide precipitation.
This is where conventional ion exchange returns. A chelating resin with iminodiacetic or aminophosphonic groups removes residual magnesium and calcium down to sub-mg/L, and a strong acid cation resin in the hydrogen form can convert the chloride solution to the acid form needed for bipolar membrane electrodialysis. Boron, which is a damaging impurity in battery-grade lithium carbonate, is removed on a dedicated boron-selective resin with N-methylglucamine functional groups. These polishing steps are small in volume but decisive for product quality.
The comparison with evaporation is worth stating plainly. Conventional solar evaporation produces lithium from brine at low operating cost but takes 12-24 months of residence time, loses 40-60 percent of the lithium to the mother liquor and to entrainment, and is only feasible in regions with high net evaporation. Direct lithium extraction, using selective adsorbents, recovers 70-90 percent of the lithium in hours rather than months and works in colder or wetter climates. The trade is capital and reagent cost against recovery and speed, and the balance has shifted toward direct extraction as lithium prices and permitting constraints have risen.
For anyone specifying materials, three numbers decide the outcome. The first is the working capacity in milligrams of lithium per gram of adsorbent per cycle, which sets the bed size. The second is the acid consumption per kilogram of lithium eluted, which sets the operating cost. The third is the capacity retention after 1000 cycles, because a material that loses 1 percent per cycle is finished in three years. Datasheets rarely give the third number, and it is the one that separates a viable project from a pilot plant that never scales.